Schmidt Hammer (Rebound Hammer) Testing

Use rebound readings to compare concrete surfaces, investigate differences and choose where further testing may help.

Table of contents

The Schmidt hammer, also called a rebound hammer or concrete test hammer, is a hand-held, non-destructive tool that measures the surface hardness of hardened concrete. A spring-driven mass strikes a plunger held against the concrete, and the distance it bounces back is recorded as the rebound number.

It is a quick, portable way to compare near-surface response across a structure. On Australian sites, it is used to map uniformity, locate weak zones, target core locations and check early strength in precast yards.

What it cannot do on its own is give a reliable compressive strength. Rebound number reflects near-surface hardness, rather than a fixed depth of concrete, and it is affected by surface condition, moisture, carbonation and aggregate type. In-situ strength estimates need a suitable project-specific correlation against cores; laboratory-cylinder curves are not automatically transferable to the structure.


At a glance: a rebound hammer compares surface response. Its number is not MPa. Use a suitable project-specific core correlation for strength estimates and the specified assessment method for decisions.

Rebound hammer test result

Terms Explained

Term Meaning
Rebound number (R) An instrument reading describing rebound behaviour. It has no MPa unit and is not itself a concrete strength.
Q-value A different rebound measure used by some digital instruments. It must not be mixed with R-values or an R-value correlation.
Correlation A relationship established from paired rebound readings and direct strength tests for the concrete being assessed.
Calibration and anvil check Instrument calibration/verification concerns the hammer’s response. A strength correlation concerns the concrete. Passing an anvil check does not validate a strength conversion curve.
Carbonation A reaction with carbon dioxide that can harden an older concrete surface and raise rebound readings without an equivalent increase in internal strength.
Laitance A weak surface layer rich in fine particles; it can distort the reading.
Outlier A reading treated differently under the chosen method’s processing rules. A low reading is not automatically an outlier.
NDT Non-destructive testing: investigation without removing a major specimen. Surface preparation can still leave visible marks.

Standards Used in Australia

There is currently no Australian Standard test method in the AS 1012 series for rebound hammer testing. Australian laboratories and consultants use international methods, normally named in the project specification or the engineer's brief.

Standard Notes
ASTM C805/C805M Rebound number of hardened concrete; widely used in Australia. States that the method is not suitable as the basis for acceptance or rejection of concrete
EN 12504-2:2021 Testing concrete in structures, determination of rebound number (Type N hammer)
ISO 1920-7 Non-destructive tests on hardened concrete, including rebound hammer
BS 1881-202 Older British recommendations, still referenced in some documents
EN 13791 Assessment of in-situ compressive strength, including how to calibrate indirect tests against cores
AS 1012.14 Cores used to calibrate rebound results (see Concrete Core Testing)

Because the method isn't in AS 1012, check whether the laboratory's NATA scope covers the international method being used, if a NATA-endorsed report is needed.

Types of Rebound Hammer

Type Impact Energy Typical Use
Type N About 2.2 N·m Standard hammer for structural concrete at least 100 mm thick
Type L About 0.74 N·m Thin or small elements, brittle materials, and rock testing
Digital / "Silver Schmidt" type Varies Electronic rebound (Q-value) with data logging; reduces reading error
Pendulum hammers Low energy Very soft or low-strength materials

The Type N hammer is the default for building and civil concrete.

When to Use a Schmidt Hammer

Good uses

  • Assessing the uniformity of concrete across slabs, walls, columns and precast units
  • Finding weak or poorly compacted zones for further investigation
  • Choosing core locations before an AS 1012.14 coring program
  • Comparing a suspect pour with a known-good pour of the same mix
  • Early-age strength checks in precast yards, against a calibration developed for that mix
  • Condition surveys of existing structures, alongside visual inspection, cover and carbonation testing
  • Field estimation of rock strength (Type L hammer) in geotechnical work

Poor uses

  • Accepting or rejecting concrete on its own
  • Replacing cylinder or core testing for compliance
  • Testing concrete under 100 mm thick, or members that move under impact
  • Comparing different mixes, ages or surface finishes without separate calibration
  • Testing very young concrete that marks under the plunger

Procedure

The steps below reflect common practice under ASTM C805. Follow the method named in the specification.

1. Verify the Hammer

Check the hammer on its steel test anvil before and after each testing session. Use the reference value and tolerance for the specific hammer and anvil, not a universal rebound number. If the check fails, stop and follow the manufacturer’s verification or servicing process.

2. Select and Prepare the Test Area

  • Concrete at least 100 mm thick and fixed within the structure
  • Test area at least about 150 mm in diameter
  • Grind off loose mortar, laitance, paint, render and heavily trowelled skin with an abrasive stone
  • Avoid honeycombing, scaling, exposed aggregate and areas directly over reinforcement near the surface
  • Note whether the surface is formed, trowelled or ground, because each gives different readings

3. Hold the Hammer

Hold the hammer perpendicular to the surface. Push slowly until the hammer releases. Record the rebound number and the hammer orientation (horizontal, vertically up, vertically down or inclined), because gravity affects the rebound.

4. Take Readings

  • Take the number of readings per test area that the specified method requires, spaced apart and away from edges
  • ASTM C805 and EN 12504-2 set different numbers and spacings, so follow the one named in the specification
  • Don't test the same spot twice

5. Process the Readings

Apply the averaging or median calculation and outlier/retest rules in the specified edition. ASTM and EN procedures differ; do not combine their rules. Keep all readings, identify excluded readings with reasons, and report the statistic required by that method.

Arithmetic example only: readings 30, 31, 31, 32, 32, 32, 33, 33, 34 and 34 have a mean of 32.2 and median of 32. These are rebound numbers, not MPa, and no concrete strength can be assigned without a suitable correlation.

6. Record Supporting Information

  • Element, location and grid reference
  • Hammer type, serial number and anvil check result
  • Surface condition and preparation
  • Moisture condition (dry, damp, wet)
  • Orientation of the hammer
  • Age of the concrete, where known
  • Carbonation depth, if measured

Factors That Affect the Rebound Number

Factor Effect
Surface texture Rough or honeycombed surfaces give low readings; hard-trowelled surfaces read high
Moisture Wet surfaces give lower readings than dry
Carbonation Carbonated surface layers are harder, giving higher readings on older concrete
Aggregate type Different aggregates give different rebound for the same strength
Cement type and age Change the rebound–strength relationship
Orientation R-value hammers require the manufacturer’s impact-angle correction; Q-value instruments may be angle-independent. Follow the particular instrument’s instructions
Element stiffness and thickness Thin or flexible elements absorb energy and read low
Reinforcement near the surface Testing directly over a bar reads high
Temperature Frozen concrete reads high

Because so many factors are involved, the manufacturer's generic conversion curve on the side of the hammer is not reliable for estimating strength on its own.

Estimating Strength: Calibrate Against Cores

To estimate in-situ compressive strength:

  1. Carry out a rebound survey across the elements in question.
  2. Choose core locations covering the range of rebound values, from lowest to highest. ASTM C805 calls for at least two replicate cores from at least six locations to build a correlation.
  3. Take rebound readings at each core location before drilling.
  4. ASTM C805/C805M-25 calls for cores tested to ASTM C42/C42M. If an Australian project instead uses AS 1012.14, obtain approval for that adapted correlation protocol and document the difference; do not describe it as unmodified ASTM compliance.
  5. Plot core strength against rebound number and fit a project-specific relationship.
  6. Use that relationship, with its scatter, to estimate strength at the other test locations.

EN 13791 sets out a formal procedure for this calibration and for estimating in-situ characteristic strength from combined core and indirect test data.

Laboratory cylinders may not reproduce the moisture, texture and carbonation of the structure’s surface. A cylinder-derived curve is not automatically transferable to in-situ concrete.

A simple calibration is often linear over the range tested:

Estimated strength = a × R + b

Here, R is rebound number; a is the fitted slope and b the fitted intercept. This is an example relationship, not a universal conversion.

where R is the rebound number, and a and b are fitted from paired core and rebound results for that concrete only.

Interpreting a Rebound Survey

Even without strength calibration, a rebound survey is very useful for comparison:

Observation What It May Indicate
Uniform readings across an element Consistent concrete and compaction
A zone reading well below its surroundings Poor compaction, segregation, a different load, or early-age damage
Low readings near the tops of walls and columns Normal bleed and compaction gradient, unless excessive
High readings on old concrete Often carbonation rather than higher strength
Large scatter within one test area Rough surface, aggregate near the surface, or operator technique

Plotting results on a grid or contour map of the element is the clearest way to present a survey.

Example: A Low-Reading Patch

Suppose one wall area has a rebound statistic of 28 and adjacent areas read about 36 under the same adopted method. The lower figure identifies a difference to investigate; it does not mean the wall is “28 MPa concrete”.

First compare moisture, finish, orientation, age, stiffness and reinforcement proximity. Map the areas and retain all individual readings. If a material difference remains plausible, the engineer can select core locations and an appropriate assessment protocol. Where strength is estimated from a correlation, state its calibration range and uncertainty; avoid extrapolating beyond the paired data.

The useful deliverable is usually a location plan with test-area statistics, surface observations and follow-up recommendations. An isolated strength number copied from the hammer’s generic chart hides the information needed to interpret the survey.

Schmidt Hammer and Other NDT Methods

Rebound testing is often combined with other non-destructive tests for a more reliable picture.

Method What It Adds
Ultrasonic pulse velocity (UPV) Measures travel time along a defined sound path; can help investigate uniformity and defects, depending on access and test arrangement
SonReb (rebound + UPV) Combined correlation, often more reliable than either method alone
Covermeter / GPR Locates reinforcement before testing and coring
Carbonation testing Explains high rebound on older surfaces
Cores Direct strength measurement for calibration

Advantages and Limitations

Advantages

  • Fast, cheap and portable
  • Non-destructive
  • Hundreds of readings per day across a structure
  • Good for comparing areas and targeting cores

Limitations

  • Responds to near-surface hardness; there is no universal 30 mm test depth
  • Strongly affected by surface, moisture, carbonation and aggregate
  • Generic strength curves are unreliable
  • Not suitable for concrete acceptance
  • Needs calibration against cores for any strength estimate

Is there an Australian Standard for the Schmidt hammer?

There is no current AS 1012 method for rebound hammer testing. Australian practice uses ASTM C805, EN 12504-2 or ISO 1920-7, as named in the specification.

Can a Schmidt hammer tell me the strength of concrete?

It measures rebound response. A defensible in-situ strength estimate needs a suitable correlation and its uncertainty; a generic chart alone is inadequate for a project strength decision.

How many readings should I take?

Follow the adopted method and edition: ASTM C805 uses 10 readings per test area; EN 12504-2 uses at least 9. Their processing and rejection rules differ. Preserve the complete raw set and apply the chosen method’s rules.

Can I use a Schmidt hammer to accept concrete?

No. ASTM C805 explicitly states the method is not suitable as the basis for acceptance or rejection. Use cylinders, and cores where needed.

What is the difference between Type N and Type L hammers?

Type N has about three times the impact energy of Type L. It is used for normal structural concrete. Type L is for thin elements, brittle materials and rock.


Sources and Method Scope

This learning guide explains purpose, terminology and interpretation. It is not the full test method. Use the project-adopted standards, amendments, specification and controlled laboratory procedure for exact apparatus, timing, conditioning, calculations and decision rules.