Concrete core testing means drilling cylindrical samples out of hardened concrete and crushing them in a laboratory to estimate the strength of the concrete in the structure. It is the standard method in Australia when cylinder results are low, missing or disputed, or when an existing structure needs to be assessed.
Cores are secured, prepared and tested in accordance with AS 1012.14 (Method for securing and testing cores from hardened concrete for compressive strength and mass per unit volume). This guide refers to AS 1012.14:2018; use the edition and amendments adopted for the investigation. The crushing itself follows AS 1012.9, and density follows AS 1012.12.1 or AS 1012.12.2.
Core testing is a structural assessment tool. Because core strengths are more variable than cylinder strengths and are affected by drilling, position and curing history, they are not used for routine quality control of concrete supply.
At a glance: a core is drilled from the structure, prepared, conditioned and tested. The engineer must plan both the sampling and interpretation; scanning, drilling release and repair are part of the job.
Terms Explained
| Term | Plain-English meaning |
|---|---|
| In situ | In its original position in the structure, rather than in a separately moulded specimen. |
| Core | A cylinder drilled out of hardened concrete; it carries the structure’s actual compaction, exposure and curing history. |
| L/d ratio | Prepared core length divided by its diameter. The specimen’s proportions affect the measured strength. |
| Conditioning | Bringing the core to the moisture and temperature state required by the selected method before testing. |
| Corrected core strength | Measured core strength adjusted using the correction allowed by the method. It is not automatically an equivalent standard-cured cylinder strength. |
| Honeycombing | Voids or stone pockets where mortar has not fully filled the concrete, often associated with placement or compaction problems. |
| GPR and covermeter | Ground-penetrating radar and electromagnetic reinforcement-location equipment. They assist scanning but have detection and interpretation limits. |
| Carbonation | A reaction with atmospheric carbon dioxide that lowers concrete alkalinity. It can affect reinforcement protection and surface-hardness measurements. |
When Core Testing Is Useful
- Cylinder results for a pour are below the specified strength
- Cylinders were never taken, were lost or were damaged
- There is a dispute between the builder, supplier and client over concrete quality
- An existing building, bridge or wharf is being assessed for refurbishment, change of use or added load
- Fire, impact, flooding or chemical attack has damaged the concrete
- Honeycombing, poor compaction or segregation is suspected
- Durability testing is needed, such as carbonation depth, chloride profile or sulfate content (these use the core but are separate tests)
- A forensic investigation into cracking or failure
Choose the Sampling Plan to Match the Question
An investigation of a visibly defective patch is different from estimating strength across an entire floor. Cores targeted at the worst-looking concrete can help define a defect, but their average does not represent the whole pour. Cores selected only from convenient locations can also bias the assessment.
Before booking, give the engineer and laboratory the element drawings, original cylinder reports, pour boundaries, approximate concrete age, access restrictions and suspected defect locations. Agree the assessment zones, sampling basis, spare locations, conditioning and decision criteria. Include scanning, drilling access, reinstatement and interpretation in the scope—not just the price of each laboratory test.
Australian Standards and Guidance
| Standard / Document | Relevance |
|---|---|
| AS 1012.14:2018 | Securing, preparing, conditioning and testing cores; L/d correction; rejection criteria; interpretation guidance in Appendix A |
| AS 1012.9 | Compressive strength test and calculation of area |
| AS 1012.12.1 / 1012.12.2 | Mass per unit volume of hardened concrete |
| AS 1012.20 | Chloride and sulfate in hardened concrete (often run on cores) |
| AS 3600 | Design strength assumptions the core results are compared against |
| AS 5100.7 | Bridge assessment |
| CIA Z11-2002 | The Concrete Institute of Australia's former recommended practice on evaluating strength from cores; withdrawn in 2016 |
| BS EN 13791:2019 / BS 6089:2010 | Assessment of in-situ compressive strength; the Concrete Institute has pointed to these as references in place of Z11 |
AS 1012.14 sets out how to get a reliable core strength. It does not set a pass/fail criterion for the structure. That judgement belongs to the structural engineer, using the project specification, AS 1012.14 Appendix A and recognised guidance.
Before drilling...
- Agree the investigation plan. The structural engineer defines the question, assessment criteria, locations and number of cores. Targeted samples from suspect zones and representative samples answer different questions; record the sampling basis.
- Release a drilling hold point. Approve each hole’s position, diameter, depth and rig fixing method, considering the element’s structural role and the proposed repair.
- Locate reinforcement, PT tendons and services. Review drawings and use a competent scanning operator. GPR and covermeters have detection limits: a scan is not a guarantee of clearance. Resolve uncertain targets before drilling. PT work needs the PT/structural designer’s approval.
- Control services and access. Arrange required service isolation and verification, secure the rig, protect the underside from falling cores and slurry, and establish exclusion zones.
- Control drilling hazards. Use the site’s silica dust controls, suitable water/electrical protection, slurry collection and disposal, and noise and eye protection. Wet drilling alone is not a complete risk control plan.
- Specify the repair. The engineer-approved repair must restore the required structural, durability, waterproofing and fire performance. Filling a hole with generic non-shrink grout is not automatically adequate.
Core Size
AS 1012.14 sets requirements for core diameter relative to the nominal aggregate size, and limits on how short a core can be relative to its diameter. In practice:
| Consideration | What It Means in Practice |
|---|---|
| Diameter | 100 mm cores suit most concrete with 20 mm aggregate; larger aggregate needs a larger core |
| Length | Aim for a core about twice as long as its diameter; a short core gives a less reliable result and may be liable to rejection |
| Consistency | The core should be a uniform, straight cylinder along its length |
| Direction | Perpendicular to the surface where possible; the direction is recorded |
Smaller cores can be more variable. Agree the number and size with the engineer and laboratory under the adopted method; do not assume that a larger number of undersized cores makes an invalid sampling plan acceptable.
Core Testing Procedure
1. Drill the Core
Drill with a water-cooled diamond core barrel, held rigidly so it doesn't wander. Record the location, element, drilling direction and date. Mark each core with its identification and orientation (outer surface end).
2. Inspect and Log
Photograph and log each core:
- Length as drilled
- Voids, honeycombing, cracks, cold joints
- Aggregate distribution and any segregation
- Reinforcement intersected (size, position)
- Carbonation depth, if separately requested, using an agreed fresh surface or separate sample so the strength specimen’s preparation is not compromised
3. Trim the Ends
Saw the ends square and parallel. Remove the outer surface layer and any reinforcement if possible while keeping an adequate length.
4. Check for Rejection
A core can be liable to rejection under AS 1012.14 if, for example, it is too small for the aggregate, too short for its diameter, has broken edges or ends that are out of square or not flat, or has a defect likely to affect the result. The method sets the limits, and it allows some cores to be re-trimmed rather than discarded.
5. Condition the Core
Agree the conditioning regime under AS 1012.14:2018 before testing. The laboratory must apply the prescribed moisture condition, temperature, humidity and duration, and report the conditioning used. Do not shorten conditioning to meet a reporting deadline. Moisture condition affects strength, so compare results only with that context.
6. Measure, Cap and Test
Measure two diameters at right angles near each end and at the centre. Area is calculated from the centre diameter, as in AS 1012.9. Grind, saw or bond-cap the ends; unbonded rubber caps are not used on cores. Then crush in the compression machine as for cylinders.
7. Calculate the Core Strength
The core strength is the maximum force divided by the cross-sectional area:
Measured core strength (MPa) = maximum force (N) ÷ loaded area (mm²).
A core shorter than about twice its diameter tends to test stronger than a longer one, because the platens restrain more of it. AS 1012.14 therefore applies a length-to-diameter correction to give a corrected strength. The correction reduces the strength of shorter cores and makes no change to a core of standard proportions. Both the measured and the corrected strength are reported, rounded as the method specifies.
Illustrative calculation
A 100 mm core (centre diameter 99.6 mm) is trimmed to 150 mm long and fails at 230.0 kN.
Area = π × 99.6² ÷ 4 ≈ 7,791 mm².
Uncorrected core strength = 230,000 N ÷ 7,791 mm² ≈ 29.5 MPa, before the method’s geometry correction and reporting rule.
Its length is about 1.5 times its diameter, so the correction factor from the method is applied to this value to give the corrected strength.
Interpreting Core Results
A core strength is not the same thing as a standard cylinder strength. The main reasons they differ are:
| Factor | Effect on Core Strength |
|---|---|
| In-situ curing (less ideal than lab curing) | Usually lower |
| Compaction in the element | Lower near tops of walls, columns and deep pours |
| Drilling damage and micro-cracking | Lower, more so for small cores |
| Reinforcement in the core | Unpredictable; avoid or reject |
| Core direction relative to casting direction | Horizontal cores often lower than vertical |
| Moisture condition at test | Wet cores lower than dry |
| Age of concrete | Older concrete is often stronger than its 28-day value |
Because of these factors, in-situ core strength is commonly expected to be lower than the standard-cured cylinder strength of the same concrete.
Common Assessment Approach
There is no single Australian pass/fail rule for cores. For context, an ACI 318 investigation provision uses the following criteria within its own scope; these are not default Australian acceptance criteria or a complete structural assessment:
- The mean of a set of cores is compared with a proportion of f′c, and
- Each individual core is compared with a lower proportion of f′c
Some Australian specifications adopt similar criteria. Others require an engineer to estimate an equivalent in-situ characteristic strength using the guidance in AS 1012.14 or EN 13791 / BS 6089 statistical methods. Always use the criteria named in the project specification. If none are named, agree the method with the structural engineer before cores are taken.
Under AS 1379, concrete supplied that failed to conform on cylinder results is generally not made conforming by later core results. Cores answer a different question: is the structure adequate for its purpose?
Reporting
A complete core test report should include:
- Core identification, element and location (with a marked-up drawing)
- Date drilled and date tested
- Drilling direction
- As-drilled length, trimmed length and diameters
- L/d ratio and correction factor
- The actual conditioning procedure, duration and moisture condition required by the adopted method
- End preparation method
- Visual description, voids and reinforcement present
- Mass per unit volume and method used
- Core strength and corrected strength
- Any reason a core was liable to rejection
- NATA endorsement where applicable
Mistakes to avoid
- Coring without scanning for reinforcement or PT tendons
- Drawing conclusions from too few cores or from a biased sampling plan
- Cores that are too short for their diameter
- Using small 50 mm cores in 20 mm aggregate concrete
- Leaving reinforcing bar in the test specimen
- Not reporting the moisture conditioning
- Comparing core strengths directly with f′c without considering in-situ factors
- Not agreeing the assessment criteria before drilling
Managing Core Results in a LIMS
A LIMS keeps a core's chain of records: where and how it was drilled, its inspection and any reason it is liable to rejection, its conditioning time, its dimensions and strength, and who checked the result. Cores are not part of our worked example, but the same review and reporting steps apply: see Part 7: Review and approve and Part 8: Report and assess of Concrete Testing in a LIMS. Whatever system you use, verify the configured method, calculation rules and report wording against the laboratory’s controlled procedure; software output does not itself establish standards compliance or authorise construction work.
How many cores do I need?
The engineer sets the number for the investigation and assessment method. Three cores may form a set under some criteria, but three is not a universal minimum that makes a zone adequately assessed. Allow for variability, rejected specimens and the size and significance of the area.
What diameter core should be used?
100 mm is usual for 20 mm aggregate concrete. AS 1012.14 sets a minimum diameter that increases with the nominal aggregate size, so concrete with larger aggregate needs larger cores.
Are core results lower than cylinder results?
Usually, yes. In-situ curing, compaction, drilling damage and moisture condition all tend to lower core strength compared with standard-cured cylinders of the same concrete.
Can cores be used to accept concrete that failed on cylinders?
They can show the structure is adequate, but they don't change the cylinder non-conformance under AS 1379. Acceptance is a contractual and engineering decision.
Is core testing destructive?
Yes. It removes material and leaves a hole requiring an approved repair. Review drawings, scan and obtain the drilling release first; scanning reduces uncertainty but does not guarantee that reinforcement, tendons or services will be avoided.
How long does core testing take?
Allow for access approval, scanning, drilling, specimen preparation and the full conditioning period required by the nominated method. Ask the laboratory to confirm the reporting date after the conditioning regime is agreed.
Sources and Method Scope
This learning guide explains purpose, terminology and interpretation. It is not the full test method. Use the project-adopted standards, amendments, specification and controlled laboratory procedure for exact apparatus, timing, conditioning, calculations and decision rules.
-
Standards Australia — AS 1379:2026 catalogue entry; obtain the project-adopted standards and amendments for detailed requirements