Concrete Compressive Strength Testing (AS 1012.9)

Read a cylinder strength report, calculate MPa, and understand what low results mean for supply conformity and the structure.

Table of contents

A concrete compression test measures how much squeezing stress a specimen can resist. A laboratory crushes cylinders moulded from fresh concrete at planned ages, often 7 and 28 days. The results help assess whether the delivered concrete meets the specified requirements.

In Australia the test is carried out in accordance with AS 1012.9 (Compressive strength tests – Concrete, mortar and grout specimens). The cylinders are sampled to AS 1012.1 and made and cured to AS 1012.8.1. The results are then assessed for conformity under AS 1379 (Specification and supply of concrete) and the project specification.

A cylinder result tells you about the potential strength of the concrete as supplied, cured under controlled standard conditions. It is not a direct measure of the strength of the concrete in the slab, column or wall. That distinction drives most of the confusion when results come back low.

Note on AS 1379: The Standards Australia catalogue lists AS 1379:2026 as the current edition, superseding AS 1379-2007. Many current contracts, road authority specifications and supplier agreements still cite the 2007 edition. Always check which edition your project specification calls up before applying any assessment criteria.


At a glance: cylinder tests measure specimen strength. Standard-cured results support supply assessment; early construction decisions need separately planned strength evidence. A low result starts an investigation, not an automatic verdict on the structure.

Terms Explained

Term Plain-English meaning
Compression A squeezing force. This test loads a specimen until it breaks.
MPa (megapascal) A unit of stress: 1 MPa = 1 newton per square millimetre (N/mm²). Force alone is not strength; the loaded area matters.
f′c (characteristic strength) The specified concrete strength, usually at 28 days. It is a statistical value with a defined lower-tail probability, commonly 5%, rather than the average of two cylinders.
Batch, sample and specimen A batch is a quantity mixed together; a sample is concrete collected under the sampling method; a specimen is one cylinder moulded from that sample. One sample can produce several specimens.
Companion cylinders Cylinders made from the same sample and tested at the same age. Their agreement helps identify problems with specimens or testing.
Curing Controlling moisture and temperature while concrete hardens. Standard curing and curing intended to represent the structure serve different purposes.
Conformity Meeting the supply standard and project requirements, assessed using the specified grouping and decision rules.
NATA The National Association of Testing Authorities, Australia. Accreditation covers specified activities; check the laboratory’s scope for the sampling, specimen-making and testing work required.

What Compressive Strength Testing Tells You

The test measures the compressive strength of a specimen at a stated age. Conformity is assessed from the required set of results under the adopted supply standard and specification; one cylinder result does not establish characteristic strength.

Concrete in Australia is specified by strength grade, for example N32 (normal-class, 32 MPa) or S40 (special-class, 40 MPa). The number identifies the specified characteristic compressive strength in MPa, usually at 28 days. The N or S prefix describes the supply class, not a cylinder’s measured result. Confirm the grades, default properties and test age in the adopted edition and purchase specification.

Compressive strength results are used to:

  • Confirm conformity of the concrete supplied with AS 1379 and the specification
  • Track supplier performance across a project
  • Decide when formwork can be stripped, props removed or tendons stressed (early-age tests)
  • Trigger an investigation when results fall short
  • Support structural design assumptions under AS 3600 or AS 5100.5

Which Question Are You Trying to Answer?

Your question Evidence to arrange What the result means
Did the delivered concrete meet the supply requirements? The specified sampling plan and standard-cured specimens Input to AS 1379 and project conformity assessment
Can this element be stressed, stripped or loaded today? Separate early-age specimens under an approved representative curing plan, or an approved alternative Strength evidence for the named release authority
Is concrete already in the structure adequate? An engineer-led investigation, with cores where justified In-situ assessment of the structure

Example: companion results of 35.0 and 37.0 MPa have an arithmetic mean of 36.0 MPa. Where the adopted rules permit that grouping, it can become a sample result. It does not establish the characteristic strength of the entire pour. Keep the individual results, test age, curing record and applicable assessment rule with the mean.

Australian Standards for Compressive Strength Testing

Standard What It Covers
AS 1012.1 Sampling of fresh concrete
AS 1012.8.1 Making and curing compression and indirect tensile specimens (cylinders)
AS 1012.9 Compressive strength test on concrete, mortar and grout specimens
AS 1012.12.1 / 1012.12.2 Mass per unit volume (density) of hardened concrete
AS 1012.14 Cores from hardened concrete (see Concrete Core Testing)
AS 1379 Specification and supply of concrete, including conformity assessment
AS 3600 Concrete structures; relies on AS 1379 for concrete quality control
AS 5100.5 Bridge design – concrete
State road authority specifications e.g. TfNSW B80, TMR MRTS70, DTP (VicRoads) Section 610, DIT SA ST-SC-S7, Main Roads WA 820

If the contract requires NATA-endorsed results, confirm the laboratory’s scope covers the particular test and relevant field activities before booking. See the accreditation note below.

Test Specimens

Cylinder Sizes

Cylinder Size (Diameter × Height) Typical Use
100 × 200 mm The standard specimen for most structural concrete in Australia
150 × 300 mm Concrete with larger aggregate, mass concrete, some road and bridge work

The 100 × 200 mm cylinder is used on almost every building and civil project because it is lighter, needs less concrete and uses a smaller machine. Specimen size has a small effect on measured strength, so you shouldn't mix sizes when comparing results for the same mix.

How Many Cylinders Per Sample

A sample is concrete collected according to AS 1012.1; a delivery load can contain more than one production batch. Several cylinders are moulded from each sample. The following is a planning example, not a prescribed minimum:

Cylinders Test Age Purpose
1 7 days Early indication of strength development
2 28 days Conformity result (the sample strength is the mean of the pair)
1 (optional) Held as spare Retest or 56-day result if permitted

Post-tensioned, precast and fast-track work usually adds early-age cylinders at 1, 2, 3 or 4 days (see Post-Tension Early Age Testing).

How the Test Is Carried Out

1. Sample the Concrete (AS 1012.1)

Take the sample from the truck discharge after the first portion of the load has been placed, not from the very first or last concrete out of the chute. Record the docket number, truck, batch time, time of sampling, any water or admixture added on site, and the pour location.

Measure the slump from the same sample (see Concrete Slump Testing).

2. Mould the Cylinders (AS 1012.8.1)

  • Use clean, oiled, rigid moulds that are watertight
  • Fill in layers and compact each layer by rodding or vibration as the standard requires
  • Strike off the top flush and level
  • Label each cylinder with a unique identifier that links back to the sample record

3. Initial Curing on Site

Keep specimens undisturbed and protected from moisture loss, temperature extremes, vibration and damage. Provide the temperature control, curing duration and transport arrangements required by AS 1012.8.1. Record the actual curing conditions and any departures; shade alone does not establish compliant curing. Early-age specimens for construction release have a different curing purpose from standard-cured conformity specimens.

4. Standard Moist Curing in the Laboratory

The laboratory demoulds the cylinders and places them in moist curing, in lime-saturated water tanks or a fog room, at the standard temperature AS 1012.8.1 sets for the climatic zone, which is higher in tropical zones. The temperature is checked and recorded, because curing temperature affects strength gain.

5. Prepare the Ends

The ends must be flat and perpendicular to the axis so the load is applied evenly. AS 1012.9 allows several methods:

  • Unbonded rubber caps in steel retainers (the most common method in Australian laboratories)
  • Sulphur or cement-based capping compounds
  • Grinding the ends flat

The cap type is reported because it can affect the result, particularly for high-strength concrete.

6. Measure and Weigh

Measure two diameters at right angles and the height. A cylinder that is too short for its diameter, or out of shape, is liable to rejection under AS 1012.9. Many laboratories also weigh the cylinder and report the mass per unit volume to AS 1012.12.1. A density well below the expected value warrants investigation of compaction, air content, material identity and the measurement; it does not identify the cause on its own.

7. Crush the Cylinder

Place the cylinder centrally in a calibrated compression machine and load it continuously, without shock, at the steady rate of stress increase set by AS 1012.9, until failure. Loading too fast tends to raise the result, and too slow to lower it. Record the maximum force and the type of fracture.

8. Calculate the Strength

Compressive strength = maximum force ÷ loaded area

For a cylinder: area = π × mean diameter² ÷ 4.

where:

  • strength is the compressive strength in MPa (N/mm²)
  • maximum force is the maximum force in N
  • mean diameter is the mean of the two measured diameters in mm

The result is rounded as AS 1012.9 specifies, from the unrounded value.

Worked example

A 100 × 200 mm cylinder with a mean diameter of 100.2 mm fails at 285.0 kN.

Area = π × 100.2² ÷ 4 ≈ 7,885 mm².

Strength = 285,000 N ÷ 7,885 mm² ≈ 36.1 MPa before applying the method’s reporting rule.

Reading Fracture Patterns

Record the fracture pattern and review it alongside end preparation, alignment, machine performance, specimen condition and curing records. A normal cone fracture is not proof that a result is reliable. An abnormal fracture is a reason for technical investigation, not automatic permission to discard a low result. Retain the raw result and document any decision under the governing method.

7-Day vs 28-Day Strength

The specified test age governs conformity, commonly 28 days. A 7-day result is usually an early indicator, unless the contract separately specifies a 7-day requirement.

For some general-purpose (GP) cement mixes, 7-day strength may be about 65–75% of the mix’s eventual 28-day strength. This is not 65–75% of the specified grade, and is not a universal acceptance band. Cementitious materials, temperature and curing change the relationship.

Illustrative example: if supplier data for a particular mix indicates an expected 28-day strength of 40 MPa, a 65–75% development ratio would correspond to 26–30 MPa at 7 days. Neither value determines conformity on its own. Use validated development data for the actual mix and follow any project-specific early warning trigger. A later test age replaces the specified conformity age only when expressly permitted.

How Results Are Assessed Under AS 1379

Concrete conformity in Australia has two layers.

Production assessment is carried out by the supplier across its plant's output for each grade. Normal-class concrete is generally accepted on the basis of the supplier's production assessment.

Project assessment is testing carried out for a specific project, usually by an independent NATA laboratory, when the customer or specification requires it. It is normally required for special-class concrete and on most civil, road and major building work.

Sample Strength

Use the specimen grouping and calculation rules in the edition of AS 1379 adopted by the contract. Investigate large differences between companion cylinders. Preserve every raw result and record the technical basis for any exclusion; never discard a result simply because it lowers the average. A summary cannot substitute for the edition-specific exclusion provisions.

Project Assessment Criteria

Identify whether production assessment, project assessment or both are required. Apply the adopted edition’s sample, moving-average and investigation criteria together with the project specification. Do not use “every result ≥ grade” as a universal acceptance rule. AS 1379:2026 superseded the 2007 edition, but a contract may still adopt the earlier edition. Resolve the governing edition before calculating conformity.

Sampling Frequency

Sampling frequency comes from AS 1379 and the project specification. Road authority specifications often set their own rates, typically a minimum number of samples each day that rises with the number of trucks supplied (DIT SA's ST-SC-S7 is one example).

Record the number of cylinders at each age in the approved plan. One 7-day and two 28-day specimens are a common arrangement, but early-age, later-age or reserve testing can require more specimens.

What to Do When Results Are Low

A low cylinder result doesn't automatically mean the concrete in the structure is deficient. Work through the evidence in order.

  1. Check the test. Review fracture type, cap type, cylinder dimensions and density, pair difference and the lab's curing records.
  2. Check the sampling and site curing. Look for cylinders left in the sun, disturbed, frozen, transported early or poorly compacted.
  3. Check the delivery. Review the docket, the time from batching to discharge, water added on site, and the slump recorded.
  4. Look at the trend. One low sample within a strong moving average is very different from a run of borderline results.
  5. Assess the structure. If doubt remains, the engineer selects an investigation proportionate to the concern. A rebound survey may help map variation and target cores; it is not a mandatory step before coring or a strength acceptance test.
  6. Engineering assessment. The structural engineer decides whether the in-situ strength is adequate for the design actions, possibly with load testing, strengthening or replacement in extreme cases.

Under AS 1379, a failure to conform is generally not reversed by later testing. Cores or rebound testing assess whether the structure is fit for purpose, not whether the concrete supplied conformed.

Common Causes of Low Cylinder Results

Cause Typical Effect
Water added on site beyond the mix design Lower strength across the batch; often shows up as a high slump
Poor compaction of cylinders Low density and low strength
High initial curing temperature or drying Reduced 28-day strength
Cylinders frozen or disturbed before setting Low and erratic results
Late delivery / long time in the agitator Slump loss, water added, lower strength
Non-parallel ends or poor capping Shear or abnormal fractures, low results
Testing machine out of calibration Systematic error across many results
Mix supplied was the wrong grade Consistently low results; check dockets

Remember...

  • Book a NATA-accredited testing laboratory before the pour
  • Agree the sampling plan, test ages and number of cylinders in the inspection and test plan (ITP); see Construction Quality Assurance
  • Record docket details and any water added for every sampled truck
  • Provide a protected, level location for cylinders on site
  • Never move cylinders before they have set
  • Make extra cylinders where early stripping, propping or stressing decisions depend on them
  • Review results as they come in, not after the 28-day results for the whole job
  • Keep 7-day results in perspective: they are an early warning, not a pass/fail

Managing Results in a LIMS

A laboratory information management system (LIMS) keeps each cylinder tied to the load it came from: its label from moulding, the curing record, the breaking session's machine checks, the strength calculated and rounded as the method specifies, the reviewer's check and the AS 1379 assessment. Our worked example follows one load's cylinders from the truck to the report, with real numbers: see Part 5: Break the cylinders and beams and Part 8: Report and assess of Concrete Testing in a LIMS. Whatever system you use, verify the configured method, calculation rules and report wording against the laboratory’s controlled procedure; software output does not itself establish standards compliance or authorise construction work.

Frequently Asked Questions

What is f′c?

f′c is the characteristic compressive strength of concrete at 28 days, in MPa. It is the strength grade number, for example 32 MPa for N32 concrete.

Why are 100 × 200 mm cylinders used instead of cubes?

Australian practice is based on cylinders under AS 1012.8.1 and AS 1012.9. Cubes are used for grout and mortar, but concrete strength grades in AS 1379 and AS 3600 are cylinder strengths. A cube result is not directly comparable with a cylinder result because cubes typically give higher values.

Can concrete pass at 7 days?

A 7-day result can satisfy a separately specified early-age requirement. It does not establish 28-day conformity. Use the age and assessment rules actually specified; later-age testing substitutes for the nominated age only where permitted.

How long does the test take?

The crush itself takes a few minutes. The result for a 28-day cylinder is usually available on the day it is tested, and NATA reports follow shortly after.

Does a higher slump mean lower strength?

Not necessarily. Slump measures consistency, not strength or water–cement ratio. Water added beyond the approved mix allowance can reduce strength, while admixtures can increase slump without that increase in water. Mix composition, air content, age and curing also affect strength.

What if one cylinder in a pair is much lower than the other?

Check the pair difference against AS 1379 and look for an assignable cause such as a damaged cylinder, poor capping or an abnormal fracture. The standard sets rules for which cylinder may be excluded.


Sources and Method Scope

This learning guide explains purpose, terminology and interpretation. It is not the full test method. Use the project-adopted standards, amendments, specification and controlled laboratory procedure for exact apparatus, timing, conditioning, calculations and decision rules.

Checking Laboratory Accreditation

Check the scope for the specific activities required, including field sampling and specimen making where relevant. NATA accreditation is activity-specific, and report endorsement applies to accredited work. See NATA’s accreditation sectors and the Australian Government’s explanation of scopes of accreditation.