Concrete testing provides evidence about the properties of the concrete supplied and built into Australian projects.
Different tests answer different questions; no single result proves all aspects of strength, durability and workmanship. Some tests check the fresh concrete at the truck: is it the right consistency, air content and temperature? Others check hardened specimens in the laboratory: did it reach its strength? A third group tests the finished structure itself.
Almost all concrete test methods in Australia are in the AS 1012 (Methods of testing concrete) series. The rules for specifying, supplying and assessing concrete are in AS 1379 (Specification and supply of concrete), and design requirements are in AS 3600 (Concrete structures) and, for bridges, AS 5100.5. State road authorities add their own specifications for roads, bridges and other infrastructure.
Start with the test’s purpose: fresh-concrete consistency, standard-cured specimen strength, in-situ investigation, or early-age construction release. A test result, supply conformity and structural adequacy are separate decisions. Use the project’s nominated decision rule and release authority.
New to concrete testing? Start with the terms below, choose the test by the decision you need to make, and use the linked guides for the detail.
Terms
| Term | Meaning |
|---|---|
| Fresh and hardened concrete | Fresh concrete can still be placed and compacted; hardened concrete has set and developed strength. |
| Cement, binder and aggregate | Cement reacts with water; binder includes cement and other cementitious materials; aggregate is the sand and stone within the concrete. |
| Sample and specimen | A sample is collected concrete; a specimen is a cylinder, beam, cube or prism made from it. Several specimens can come from one sample. |
| Strength and MPa | Strength is failure force divided by the relevant area or a stress calculated from the test geometry. MPa means N/mm². |
| f′c | Specified characteristic compressive strength, usually at 28 days. It is a statistical design/supply value, not the mean of an arbitrary group of results. |
| Curing | Maintaining the moisture and temperature conditions needed for hardening. Specimen curing must match its test purpose. |
| In situ | In the actual structure. A core reflects different conditions from a separately moulded, standard-cured cylinder. |
| ITP | Inspection and test plan: the agreed checks, frequencies, criteria, records and responsibilities for the work. |
| Conformity and structural adequacy | Conformity concerns the specified supply requirements. Structural adequacy concerns whether the constructed member can safely fulfil its purpose. |
| NATA accreditation | Recognition of competence for listed activities. Check the laboratory’s scope for the particular methods and field work required. |
Concrete Testing

| Test | Purpose | Australian Method | Guide |
|---|---|---|---|
| Compressive strength | Specimen strength used in the specified conformity assessment | AS 1012.9 | Compressive Strength Testing |
| Slump | Consistency of fresh concrete as delivered | AS 1012.3.1 (slump flow: AS 1012.3.5) | Slump Testing |
| Core testing | Strength of concrete in the structure | AS 1012.14 | Core Testing |
| Grout testing | Strength, flow and bleed of cement grouts | AS 1012.8.3, AS 1012.9, TS 02800.49 | Grout Testing |
| Flexural strength | Bending (tensile) strength for pavements | AS 1012.11 | Flexural Strength Testing |
| Air content | Total air in fresh concrete; one input to mix control | AS 1012.4.1 / 4.2 / 4.3 | Air Content Testing |
| Schmidt hammer | Surface hardness and uniformity of hardened concrete | ASTM C805 / EN 12504-2 (no AS method) | Schmidt Hammer Testing |
| Post-tension early age | Early-age strength evidence for the specified stressing release | AS 1012.8.1, AS 1012.9, AS 3600 | Post-Tension Early Age Testing |
A quick guide on where to start
| Situation | Start here | Why |
|---|---|---|
| Concrete has arrived and needs a consistency check | Slump or slump flow | A fresh test can inform action while the load is still identifiable |
| You need evidence of the supplied concrete’s strength | Cylinder testing | Standard-cured specimens feed the specified supply assessment |
| A slab is due for stressing | Early-age PT testing | Relevant curing and the approved release rule matter as much as the number |
| Existing concrete or low cylinder results need investigation | Core testing | The engineer plans an assessment of concrete in the structure |
| A pavement design specifies bending strength | Flexural testing | A cylinder grade cannot simply replace the required beam result |
| You need to track specimens and reports | Concrete testing in a LIMS | The walkthrough links each result to its source and history |
Before booking: provide the pour location and volume, mix requirements, governing standards and editions, sample frequency, specimen counts and ages, curing purpose, access arrangements and reporting contacts.
The Three Stages of Concrete Testing
1. Fresh Concrete (at the Truck)
Fresh concrete tests are done on site, on a sample taken to AS 1012.1, before or during placement. They provide information while the load can still be identified and the project can act on it before placement, where the sampling and decision process allows.
| Test | Standard | Typical Use |
|---|---|---|
| Slump | AS 1012.3.1 | Almost every pour |
| Slump flow, T500, J-ring | AS 1012.3.5 | Self-compacting concrete |
| Air content | AS 1012.4.2 (most common) | Pavements, freeze–thaw exposure |
| Mass per unit volume (fresh density) | AS 1012.5 | Yield, density checks |
| Temperature | Project specification / AS 1379 | Hot and cold weather concreting |
| Bleeding | AS 1012.6 | Mix design, special concretes |
2. Hardened Specimens (in the Laboratory)
Specimens are moulded from the same fresh sample, cured under standard conditions and tested at set ages.
| Test | Specimen | Standard |
|---|---|---|
| Compressive strength | Cylinders (AS 1012.8.1) | AS 1012.9 |
| Flexural strength | Beams (AS 1012.8.2) | AS 1012.11 |
| Indirect tensile strength | Cylinders | AS 1012.10 |
| Grout and mortar strength | Cubes (AS 1012.8.3) | AS 1012.9 |
| Drying shrinkage | Prisms (AS 1012.8.4) | AS 1012.13 |
| Mass per unit volume (hardened) | Cylinders or cores | AS 1012.12.1 / 12.2 |
3. In-Situ Testing (on the Structure)
In-situ tests check the concrete as built. They are used when specimen results are low or missing, for existing structures, and for durability and condition surveys.
| Test | Standard | Destructive? |
|---|---|---|
| Core testing | AS 1012.14 | Yes (repairable) |
| Rebound (Schmidt) hammer | ASTM C805 / EN 12504-2 | No |
| Ultrasonic pulse velocity | International methods (e.g. EN 12504-4) | No |
| Cover and reinforcement location | Covermeter / GPR | No |
| Carbonation depth | Phenolphthalein on a fresh face | Minor |
| Chloride and sulphate content | AS 1012.20 (on cores or dust) | Minor |
Typical Testing
- Before the pour: agree the mix, the test plan and the hold points in the ITP; book a NATA-accredited laboratory.
- At the truck: check the docket, then test slump (and air content where specified) on sampled trucks.
- Moulding: make cylinders (and beams or cubes where needed) from the same sample.
- Early age: test separately identified specimens under the approved representative curing regime for stressing, stripping or de-propping decisions. Use the specified ages and release authority.
- 7 days: test a cylinder as an early indication of 28-day strength.
- 28 days (or 56): test conformity cylinders; assess them under AS 1379 and the specification.
- If results are low: notify the nominated reviewer, check testing, sampling and delivery records, and have the engineer determine whether an in-situ investigation is needed. Rebound surveys and cores are options, not an automatic sequence.
Who Does the Testing?
- Concrete suppliers carry out production assessment of their mixes under AS 1379. Normal-class concrete is usually accepted on that basis.
- Independent NATA-accredited laboratories carry out project assessment for the builder, contractor or client. That is normally required for special-class concrete and most civil and road work.
- Engineers specify the testing, interpret results and decide on the adequacy of the structure.
Normal-Class and Special-Class Concrete
| Concrete Class | What It Means | Testing Implication |
|---|---|---|
| Normal-class (N) | Concrete supplied within the normal-class property limits of the adopted AS 1379 edition; N identifies the class, and the number identifies strength grade | Usually accepted on the supplier's production assessment; project assessment is optional unless specified |
| Special-class (S) | Concrete with properties different from or additional to normal-class, e.g. early age strength, low shrinkage, special aggregates, air entrainment, flexural strength | The specification must state how properties are tested and accepted; project assessment is common |
Post-tensioned concrete with an early stressing strength, pavement concrete specified by flexural strength, and air-entrained concrete are all typically special-class.
Road Authority Specifications
Road and bridge projects follow state specifications that build on AS 1012 and AS 1379, often with tighter frequencies and extra tests.
| State | Typical Concrete Specifications |
|---|---|
| NSW | TfNSW B80 (concrete work for bridges), R83 (concrete pavement base), B113 (post-tensioning) |
| Queensland | TMR MRTS70 (concrete), MRTS40 (concrete pavement base), Q-series test methods |
| Victoria | DTP (formerly VicRoads) Section 610 and related sections |
| South Australia | DIT ST-SC-S7 (supply of concrete) and related master specifications |
| Western Australia | Main Roads WA Specification 820 (concrete for structures) and others |
Which Australian Standard covers concrete testing?
The AS 1012 series covers methods of testing concrete. AS 1379 covers specification, supply and conformity, and AS 3600 covers structural design.
What is the difference between production and project assessment?
Production assessment is the supplier's ongoing testing of its plant's output for each grade. Project assessment is testing carried out for a specific project, usually by an independent laboratory, to check the concrete supplied to that job.
What should I do if concrete fails a test?
Check the test and sampling records first, then the delivery records, and look at the trend of results. Notify the responsible reviewer and follow the project’s non-conformance process. The engineer chooses any further testing needed; a rebound survey is not mandatory before cores.
Scanning and Coring Scope
Before drilling or cutting, obtain an approved hole plan, review drawings and arrange competent scanning for reinforcement, PT tendons and services. Scanning has detection limits and does not guarantee clearance. Resolve uncertain targets and obtain structural/PT approval, service controls and the required drilling release. The core testing guide explains investigation and drilling precautions; dedicated scanning and core-drilling service guides are not yet part of this collection.
Sources and Method Scope
This learning guide explains purpose, terminology and interpretation. It is not the full test method. Use the project-adopted standards, amendments, specification and controlled laboratory procedure for exact apparatus, timing, conditioning, calculations and decision rules.
- CCAA Guide to Concrete Construction (2020) — Part VIII, Section 26 gives background on testing and quality assurance.
- Standards Australia — AS 1379:2026 catalogue entry; obtain the project-adopted standards and amendments for detailed requirements
Checking Laboratory Accreditation
Check the scope for the specific activities required, including field sampling and specimen making where relevant. NATA accreditation is activity-specific, and report endorsement applies to accredited work. See NATA’s accreditation sectors and the Australian Government’s explanation of scopes of accreditation.
Related Resources
- Concrete Testing in a LIMS: one pour followed from booking to the issued reports, with real numbers
- Concrete Compressive Strength Testing
- Concrete Slump Testing
- Concrete Core Testing
- Grout Testing
- Concrete Flexural Strength Testing
- Concrete Air Content Testing
- Schmidt Hammer Testing
- Post-Tension Early Age Testing
- Concrete and Aggregate Testing for Construction
- AS 3600 Concrete Structures Design
- Construction Quality Assurance (ITPs and Hold Points)