Air content testing measures the volume of air in freshly mixed concrete, as a percentage of the concrete's volume. In Australia it matters most for slipform concrete pavements, air-entrained mixes for freeze–thaw exposure in alpine regions, and quality control where a mix's density, yield or strength looks wrong.
Australian methods are in the AS 1012.4 series:
- AS 1012.4.1 – increased-air-pressure method (reduction in concrete volume)
- AS 1012.4.2 – reduced-air-pressure method (reduction in air pressure in a chamber above the concrete), the pressure meter most commonly used on site
- AS 1012.4.3 – volumetric method (concrete dispersed in water), suitable for lightweight and porous aggregates
Air content and slump are usually checked together, on the same sample, at the point of placement.
At a glance: the test measures total fresh air as a percentage by volume. Distinguish apparent from corrected air content and use the specified sampling point. Total air alone does not prove freeze–thaw durability.
Terms Explained
| Term | Plain-English meaning |
|---|---|
| Air content | Air volume as a percentage of the fresh concrete volume. A 5% result means about 5 L of air per 100 L of concrete under the test conditions. |
| Apparent air content | The air result obtained from the meter determinations before any required correction for aggregate pores. |
| Aggregate correction factor | The contribution of aggregate pore air to the pressure-test response, determined for the relevant aggregate combination. |
| Percentage point | The difference between percentages: 4% to 5% is an increase of one percentage point, or 25% relative to the starting value. |
| Freeze–thaw exposure | Repeated freezing and thawing of wet concrete. Suitably distributed small air voids can relieve freezing-water pressure. |
| Yield | The volume of concrete produced by a batch. Fresh density helps calculate it when batch mass is known. |
| Point of placement | Where concrete enters the work, which can be downstream of the truck and pump. The sampling position affects how results are interpreted. |
Entrained Air vs Entrapped Air
Fresh concrete can contain both intentionally entrained bubbles and unintentionally trapped air. The total is useful for production control; bubble distribution matters when assessing freeze–thaw performance.
| Type | Bubble Size | Source | Effect |
|---|---|---|---|
| Entrapped air | Larger, irregular voids (typically over 1 mm) | Mixing and placing; poor compaction | Reduces strength; no durability benefit |
| Entrained air | Very small, well-distributed bubbles (tens to hundreds of microns) | Air-entraining admixture (AS 1478.1) | Improves freeze–thaw resistance, cohesion and workability; reduces bleeding |
The fresh-concrete test measures total air. It does not establish bubble spacing or the hardened air-void system needed for freeze–thaw durability. Use the specified mix qualification and any hardened-concrete verification as well.
When Is Air Content Testing Required?
Air entrainment is less common in Australia than in North America or Europe because most of the country doesn't experience freeze–thaw cycles. It is required or specified in these situations:
- Slipform concrete pavements: TfNSW R83 makes air-entraining agents mandatory in slipform paving mixes, with air content as a specified property
- Alpine and sub-alpine areas where concrete is exposed to freezing and thawing, for example in the Snowy Mountains, the Victorian Alps and central Tasmania; AS 3600 sets durability requirements for freeze–thaw exposure
- Special-class concrete where the supplier or designer uses air entrainment for cohesion, reduced bleeding or improved finish
- Investigation of low strength or low density, to check for excessive entrapped or accidentally entrained air
- Mix design trials and plant uniformity testing
It is not usually required for normal-class building concrete.
Australian Standards
| Standard | Method | Typical Use |
|---|---|---|
| AS 1012.1 | Sampling of fresh concrete | All methods |
| AS 1012.4.1 | Increased air pressure; measures the reduction in concrete volume | Pressure meters reading volume change; dense natural aggregates |
| AS 1012.4.2 | Reduced air pressure in a chamber above the concrete | The common "Type B" pressure meter used on site |
| AS 1012.4.3 | Volumetric; concrete dispersed in water | Lightweight, porous or highly absorbent aggregates |
| AS 1012.5 | Mass per unit volume of fresh concrete | Density and yield; often run alongside air content |
| AS 1478.1 | Chemical admixtures for concrete, including air-entraining agents | Admixture compliance |
| AS 1379 | Supply and conformity of specified air content | Acceptance |
| TfNSW R83 | Concrete pavement base; mandatory air entrainment in slipform mixes | NSW road pavements |
The pressure methods (AS 1012.4.1 and 4.2) are intended for concrete with relatively dense natural aggregates. For lightweight or highly porous aggregates, use the volumetric method (AS 1012.4.3).
How the Pressure Method Works (AS 1012.4.2)
The pressure meter uses Boyle's law. A sealed bowl of compacted concrete has an air chamber above it. The chamber is pumped to a set pressure, then a valve opens to connect it with the concrete. The more air in the concrete, the more the pressure drops. The gauge is calibrated to read the drop directly as air content in percent.
Equipment
- Pressure-type air meter: measuring bowl, cover assembly with air chamber, pressure gauge, pump and valves
- Tamping rod and mallet, or an internal vibrator
- Strike-off bar
- Calibration cylinder and equipment for the calibration check
Procedure
- Sample the concrete in accordance with AS 1012.1, from the same sample used for slump where possible.
- Fill and compact the bowl in layers, by rodding or vibration as required. Self-compacting concrete is placed without compaction. The method of compaction is recorded, because results depend on it.
- Strike off the surface flush and clean the rim.
- Clamp the cover assembly on and fill the space above the concrete with water through the petcocks to remove air.
- Pump the air chamber to the initial pressure line.
- Release the air into the bowl, tap the bowl to help equalise, and read the gauge.
- Repeat as the method requires. Follow AS 1012.4.2 and the meter instructions for pressure release, the second determination, agreement limits and any complete retest. Do not treat a repeated pressure cycle as interchangeable with a newly prepared test portion.
- Calculate the apparent air content from the readings, as the method sets out.
Aggregate Correction Factor
Some of the pressure drop is due to air in the pores of the aggregate rather than in the paste. Where the air content (rather than the apparent air content) is specified, an aggregate correction factor (G) is determined by testing the combined aggregates in the meter:
Air content = apparent air content − aggregate correction factor
In symbols: A = A₁ − G, with each value expressed as a percentage of concrete volume.
where:
- A is the air content of the concrete (%)
- A₁ is the apparent air content (%)
- G is the aggregate correction factor (%)
For plant production checks and mixer uniformity tests, the apparent air content alone is often enough. Results are rounded as the method specifies.
Illustrative calculation: with an apparent air content of 5.1% and an aggregate correction factor of 0.3%, the air content is 5.1 − 0.3 = 4.8%.
Reading and Acting on an Air Result
In the example above, subtracting a 0.3 percentage-point aggregate correction from 5.1% apparent air gives 4.8% air. Label the result correctly: an apparent value should not be silently compared with a limit written for corrected air content.
Before the pour, identify the specified property, target and tolerance, test method, sampling point, frequency and notification process. For a questionable reading, check the seal, gauge, compaction, test portion and correction record, then follow the method’s repeat/retest rules. Preserve the original readings and report the investigation.
If a confirmed result is outside the project limit, notify the designated person before the affected concrete is used. Any supplier adjustment and retesting must follow the approved process. More air is not automatically better: the fresh test does not show whether the hardened bubbles have the size and spacing needed for the specified exposure.
Air Content Values
| Concrete | Typical Air Content |
|---|---|
| Non-air-entrained concrete (entrapped air only) | About 1–3% |
| Air-entrained pavement concrete | Commonly about 3–6%, per specification |
| Freeze–thaw resistant concrete | Commonly about 4–8%, depending on aggregate size and exposure |
Always use the values and tolerances in the project specification.
Why Air Content Affects Strength
Air voids replace solid paste. For otherwise comparable concrete, more air often lowers compressive strength. The size of the change depends on the mix, its compaction and curing. Compare against mix trials and actual test results; do not convert a fresh-air reading into a strength penalty.
That is why air content is a useful check when:
- Cylinder densities are lower than expected
- Strength results are low across several trucks
- The supplier has changed the admixture, cement or sand
- Concrete has been pumped long distances or dropped from height
Factors That Change Air Content
| Factor | Effect on Air Content |
|---|---|
| Air-entraining admixture dose | Higher dose, more air |
| Fly ash with high carbon (loss on ignition) | Absorbs admixture, less air and more variable |
| Higher concrete temperature | Usually less air |
| More fine sand | Usually more air |
| Prolonged mixing or long haul | Can increase or decrease air |
| Pumping | Often reduces air content between the truck and the point of placement |
| Over-vibration | Removes entrained air |
| Some superplasticisers and other admixtures | Can increase or decrease air |
Because pumping and placing change the air content, specifications sometimes require testing at the point of placement rather than at the truck.
Calibration and Equipment Checks
- Calibrate the meter regularly using the calibration cylinder, as the standard requires
- Check the gauge zero and the initial pressure line before each use
- Keep the bowl rim and cover gasket clean so the seal is airtight
- Replace damaged gaskets and leaking valves
- Record the meter identification on every test
A leaking seal is one possible cause of false readings; investigate equipment and preparation together.
Common Testing Mistakes
- Testing a sample that has stood too long or been re-mixed
- Inconsistent compaction (results depend on the method)
- Not removing all air from above the concrete before pumping
- Forgetting to apply the aggregate correction factor when air content is specified
- Using a pressure meter on lightweight aggregate concrete
- Testing at the truck when the specification requires point of placement
Recording Air Content in a LIMS
A LIMS records both pressure-meter readings, how the bowl was compacted and any aggregate correction factor, then reports the air content (or the apparent air content) from the unrounded readings and flags readings that do not agree. The air meter's calibration checks sit on its equipment record. See the example in Part 3: Sample the concrete on site and the equipment checks in Part 1: Set up the laboratory of Concrete Testing in a LIMS. Whatever system you use, verify the configured method, calculation rules and report wording against the laboratory’s controlled procedure; software output does not itself establish standards compliance or authorise construction work.
Frequently Asked Questions
Do I need air-entrained concrete in Australia?
Only in specific cases, mainly slipform road pavements and alpine freeze–thaw exposure, or where the specification calls for it. Most building concrete in Australia isn't air-entrained.
What is a normal air content for concrete?
Non-air-entrained concrete usually contains about 1–3% entrapped air. Air-entrained mixes are typically specified somewhere in the 3–8% range depending on use.
Which air content method should I use?
The reduced-pressure meter (AS 1012.4.2) is most common on site. Use the volumetric method (AS 1012.4.3) for lightweight or porous aggregate concrete.
What is the difference between apparent air content and air content?
Apparent air content is the result derived from the meter readings using the nominated method. Corrected air content subtracts the applicable aggregate correction factor. Report which value was determined and whether a correction was applied.
Does air content affect strength?
It can. More air generally reduces strength when other conditions are comparable. The air result does not predict the strength of an individual load; use the specified strength tests and mix data.
Sources and Method Scope
This learning guide explains purpose, terminology and interpretation. It is not the full test method. Use the project-adopted standards, amendments, specification and controlled laboratory procedure for exact apparatus, timing, conditioning, calculations and decision rules.
-
CCAA Guide to Concrete Construction (2020) — Part VIII, Section 26 gives background on testing and quality assurance.
-
Standards Australia — AS 1379:2026 catalogue entry; obtain the project-adopted standards and amendments for detailed requirements