The slump test is the most common test carried out on fresh concrete in Australia. It takes a few minutes at the back of the truck. It tells you whether the concrete arriving on site has the consistency that was ordered, and helps identify changes that need investigation. Slump alone cannot establish whether water was added.
In Australia the slump test is carried out in accordance with AS 1012.3.1 (Determination of properties related to the consistency of concrete – Slump test). The method applies within a limit on nominal aggregate size. The measured slump is compared with the specified slump using the tolerances in AS 1379.
Slump is a measure of consistency, not strength. It is useful because a change in slump from one truck to the next usually signals a change in water content, admixture dosage, grading or time since batching. Each of those can affect strength, finishability and durability.
At a glance: slump checks fresh-concrete consistency in millimetres. Compare it with the ordered value and applicable tolerance. It cannot tell you strength or prove that extra water was added.
Terms
| Term | Meaning |
|---|---|
| Consistency | How readily fresh concrete deforms or flows. Slump measures one aspect of this behaviour. |
| Workability | How easily concrete can be placed, compacted and finished without separating. Two mixes with equal slump can have different workability. |
| Cohesion and segregation | Cohesion is the mix’s ability to stay together. Segregation is separation of coarse stone from mortar or paste. |
| Admixture | A product added to modify concrete behaviour. A water reducer or superplasticiser can increase flow without adding the same amount of water. |
| Specified slump and tolerance | The ordered slump and the permitted departure from it. The tolerance comes from the adopted supply standard and project specification. |
| SCC | Self-compacting concrete: concrete designed to flow and consolidate under its own weight without conventional vibration. |
| T500 and J-ring | T500 is the time to reach a 500 mm spread. A J-ring checks the mix’s ability to pass through a standard ring of bars. |
| Delivery docket | The supplier’s record linking a load to its mix, batch/delivery details and recorded site additions. |
What the Slump Test Measures
A cone of fresh concrete is formed in a standard mould. The mould is lifted, and the concrete subsides under its own weight. The slump is the difference between the mould height and the average height of the top surface of the slumped concrete, in millimetres. Use the Australian method’s measurement rule; measuring only the highest point can give a different answer.
- A low slump (stiff mix) suits kerb machines, slipform paving and some precast
- A medium slump suits most slabs, footings, beams and walls
- A high slump suits pumped concrete and congested reinforcement
- Concrete that flows out into a pancake is outside the slump test's range and is tested by slump flow instead
Australian Standards and Specifications
| Standard / Document | Relevance |
|---|---|
| AS 1012.1 | Sampling of fresh concrete |
| AS 1012.3.1 | Slump test |
| AS 1012.3.5 | Slump flow, T500 and J-ring for self-compacting concrete |
| AS 1379 | Specified slump, slump tolerances and acceptance of the load |
| TfNSW TS 02800.58 | Slump flow and related tests for high-workability concrete (NSW road and bridge work) |
| TMR Q478 | Visual stability index of super-workable concrete (Queensland) |
| Project specification | Target slump, testing frequency, rejection rules |
Slump Test Equipment
| Item | Function |
|---|---|
| Slump cone (mould) | A standard open-ended, cone-shaped mould with foot pieces and handles |
| Tamping rod | A steel rod with a rounded end, for compacting each layer |
| Base plate | A rigid, flat, non-absorbent and level surface |
| Scoop | For filling the mould |
| Ruler or measuring tape | To measure the slump |
AS 1012.3.1 sets the dimensions of the cone and rod. Damaged, dented or concrete-encrusted cones give unreliable results, so clean the cone after every test and check it against the method periodically.
Test Procedure
The steps below describe the general approach. AS 1012.3.1 sets the exact number of layers, compaction, timing and how the result is measured and rounded.
1. Take a Representative Sample
Sample in accordance with AS 1012.1, after the first part of the load has been discharged. Record the docket number, truck, time of batching, time of sampling and any water or admixture added on site.
2. Set Up the Cone
Dampen the inside of the cone and the base plate. Place the cone on the plate and stand on the foot pieces to hold it firmly in place.
3. Fill and Compact in Layers
Fill the cone in layers of about equal height, rodding each layer evenly over its cross-section the number of times the method specifies. The rod compacts each layer through its depth without driving hard into the layer below. Keep the top layer heaped above the rim while rodding.
4. Strike Off
Strike off the surface level with the top of the cone using the rod. Clean away any concrete that has fallen around the base.
5. Lift the Cone
Lift the cone straight up in one smooth, steady motion, without twisting or jolting. Sideways movement while lifting is a common cause of shear slumps. The whole test, from filling to lifting, is done promptly and without interruption, as the concrete stiffens with time.
6. Measure the Slump
Measure the difference between the mould height and the average height of the slumped top surface, following AS 1012.3.1. Record the shape and round as the method specifies.
True, Shear and Collapse Slump
| Slump Shape | Description | What to Do |
|---|---|---|
| True slump | Concrete subsides evenly and keeps roughly its shape | Measure and report |
| Shear slump | One side shears off and slides down an inclined plane | Repeat on another portion of the sample |
| Collapse slump | Concrete collapses and spreads out | Repeat on another portion of the sample |
If the repeat test also shears or collapses, the slump is not measured. The shape is reported instead, as AS 1012.3.1 requires. A repeated collapse can indicate a very fluid or unstable mix; check the ordered mix and applicable method before interpreting it. Repeated shear can reflect poor cohesion or testing conditions. Do not treat either shape as a valid measured slump or substitute a different test without checking the specification.
Slump Tolerances
AS 1379 allows the measured slump to vary from the specified slump by a tolerance that depends on the slump specified: the higher the specified slump, the wider the tolerance. The project specification may set its own. Know the tolerance for the slump ordered before the pour, so that each truck can be judged on the spot.
When a result is outside the tolerance, follow the adopted specification for notification, any permitted supplier adjustment and retesting, and acceptance or rejection. Do not add unauthorised water.
Using a Result at the Truck
Illustrative arithmetic: a 300 mm-high mould and an average slumped top height of 215 mm give a slump of 85 mm before method-specific rounding. Whether that result is acceptable depends on the ordered slump and applicable tolerance.
If a result falls outside the limit, identify the load and notify the person named in the inspection and test plan (ITP). Follow the specified adjustment, resampling and retesting process before the affected concrete is used. Record all results and any authorised addition; do not repeat tests until one happens to pass. The supplier should confirm whether an adjustment is permitted and within the approved mix allowance.
A slump within tolerance does not resolve a wrong mix code, excessive delivery time, segregation or an out-of-range temperature. Check the delivery and other specified properties as well.
Slump by Application
These ranges provide context only. They are not mix-selection rules or acceptance limits; pumpability also depends on grading, paste volume, equipment and placing conditions.
| Application | Usual Specified Slump |
|---|---|
| Slipform paving, kerb and gutter machines | 20–50 mm |
| Hand-placed road pavement and footpaths | 60–80 mm |
| Residential slabs and footings | 80–100 mm |
| Suspended slabs, beams and walls | 80–120 mm |
| Pumped concrete | 100–150 mm |
| Heavily reinforced or congested elements | 120–180 mm |
| Self-compacting concrete | Tested by slump flow (spread) instead |
Slump Flow for Self-Compacting Concrete (AS 1012.3.5)
Self-compacting concrete (SCC) and super-workable concrete spread out too far for a meaningful slump. AS 1012.3.5 covers these high-workability mixes, within the limits of spread and aggregate size it sets.
| Measurement | What It Tells You |
|---|---|
| Slump flow | Mean of two spread diameters at right angles, in mm; the filling ability of the mix |
| T500 | Time for the spread to reach 500 mm diameter, in seconds; the viscosity of the mix |
| J-ring | Height difference inside and outside a ring of bars; the passing ability through reinforcement |
| Visual segregation check | Whether a halo of paste or a pile of coarse aggregate forms |
If the two spread diameters are too far apart, the concrete has not spread evenly and AS 1012.3.5 requires the test to be repeated.
Specify the required slump-flow range, T500, passing ability and stability checks before testing. Each measures a different property: adequate spread alone does not demonstrate that SCC will pass reinforcement without blocking or segregation. Use the adopted authority specification for limits and the prescribed visual assessment method.
Importance
Water Added at the Truck
The most common reason for adding water on site is to raise the slump so the concrete is easier to place. Water beyond the approved mix allowance increases the water-to-cementitious-material ratio and can reduce strength and durability and increase shrinkage. An authorised addition within the designed allowance is a different situation.
AS 1379 controls how much water may be added after batching and requires it to be recorded on the delivery docket. Where a higher slump is genuinely needed, order it, or ask the supplier to adjust with a water-reducing admixture.
Slump Loss Over Time
Slump drops with time, temperature and travel distance. Hot weather, long hauls and waiting trucks all reduce slump. Retarders and good pour planning help, so test each load on arrival rather than relying on the plant's batching slump.
Consistency Between Trucks
On a large pour, a change in slump from truck to truck is an early warning. If slumps start to drift outside tolerance, talk to the supplier before more concrete is placed, not after the 28-day results.
Limitations
- It measures consistency only, not strength, durability or water–cement ratio directly
- It is not suitable for very stiff mixes (near-zero slump) or flowing mixes (collapse)
- It is not valid for concrete with very large aggregate (the method sets the limit)
- Two mixes with the same slump can place and finish very differently
- Results depend on operator technique, especially rodding and lifting
Common Mistakes
- Sampling from the first concrete out of the chute
- Not standing on the foot pieces, so concrete leaks out at the base
- Under-rodding or rodding unevenly
- Twisting or jerking the cone when lifting
- Measuring to a single high, low or centre point instead of using the average top-surface height
- Testing on a sloping, absorbent or vibrating surface
- Delaying the test while the concrete stiffens
Recording and Reporting
A slump test record normally includes:
- Project, pour location and element
- Docket number, truck number and mix code
- Time of batching, sampling and test
- Specified slump and measured slump
- Slump shape (true, shear, collapse)
- Water or admixture added on site
- Whether the slump complies with the AS 1379 tolerance
- Ambient and concrete temperature, where required
Recording Slump in a LIMS
A LIMS records each slump with its load: the docket, the sampling procedure, the time and temperatures, the shape of the slump and its result against the ordered slump's tolerance, so the field report can be issued before the trucks are forgotten. The worked example shows a slump, a slump flow with T500 and J-ring, and their records step by step in Part 3: Sample the concrete on site of Concrete Testing in a LIMS. Whatever system you use, verify the configured method, calculation rules and report wording against the laboratory’s controlled procedure; software output does not itself establish standards compliance or authorise construction work.
Frequently Asked Questions
What is a good slump for concrete?
There is no single "good" slump. It depends on the element, placing method and reinforcement. Most residential slabs use 80–100 mm, pumped concrete commonly 100–150 mm, and kerb machines 20–50 mm. Use the slump the engineer and supplier specify.
Can the slump test tell you the strength?
No. Slump only measures consistency. However, a high slump caused by added water is a strong signal that strength may be reduced.
Who should carry out the slump test?
For conformity testing, a technician working for a NATA-accredited testing laboratory. Supplier and contractor staff often perform slump checks for their own quality control.
How often is slump tested?
At least as often as strength samples are taken, and often on every truck for important pours. The project specification sets the minimum frequency.
What is the difference between slump and slump flow?
Slump measures how far a cone of concrete drops. Slump flow measures how far self-compacting concrete spreads, as a diameter. Slump flow is used when the concrete is too fluid for a meaningful slump.
Sources and Method Scope
This learning guide explains purpose, terminology and interpretation. It is not the full test method. Use the project-adopted standards, amendments, specification and controlled laboratory procedure for exact apparatus, timing, conditioning, calculations and decision rules.
-
Standards Australia — AS 1379:2026 catalogue entry; obtain the project-adopted standards and amendments for detailed requirements